低碳复合胶凝材料体系的力学性能与水化程度定量关系研究

Quantitative relationship between mechanical properties and hydration degree of low-carbon composite cementitious material systems

浏览量:

关键词:

低碳复合胶凝材料;辅助胶凝材料;化学结合水;水化机理;力学性能

Key words:

Low-carbon composite cementitious material; Supplementary cementitious material; Chemically bound water; Hydration mechanism; Mechanical property

刊期:

2026年第10期

DOI:

低碳复合胶凝材料;辅助胶凝材料;化学结合水;水化机理;力学性能

文章编号:

基金项目:

深圳市基础研究专项(自然科学基金)-基础研究一般计划项目(JCYJ20240813143004006、JCYJ20230808105109018);广东省科技创新专项项目(2023TX07G066);深圳市低碳建筑材料与技术重点实验室项目(ZDSYS20220606100406016);深圳大学研究生自主创新成果培养项目(315-000066010837)。

作者:

冯发堂1,王亚楠2,*,钟益斌1,陈 仓2,靖 谋1,张东东1,陈意良1,罗创涟3,叶 烽4

单位:

1.中电建生态环境集团有限公司,广东 深圳 518010;2.深圳大学 土木与交通工程学院,广东 深圳 518000;3.广州广检建设工程检测中心有限公司,广东 广州 510405; 4.深圳市水务工程检测有限公司,广东 深圳 518001

摘要

摘   要:水泥基材料的力学性能与水泥水化程度紧密相关,化学结合水法是纯水泥体系水化程度定量表征的常用手段。但掺入矿渣粉、粉煤灰等辅助胶凝材料(Supplementary cementitious materials,SCMs)后,胶凝体系的水化过程趋于复杂,传统化学结合水法难以直接反映复合体系的宏观力学性能。为此,本文以水泥、粉煤灰、矿渣粉和石英粉为原材料,设计了1组纯水泥体系和4组复合胶凝材料体系,研究了其水化机理及力学性能演化规律,揭示了化学结合水含量与抗压强度之间的定量关系。结果表明:与纯水泥体系相比,复合胶凝材料体系的抗压强度较低,总体而言,合理复配矿渣粉、粉煤灰与石英粉可在一定程度上改善后期抗压强度;复合胶凝材料体系的抗折强度对颗粒级配、基体密实性及裂缝扩展较为敏感;与纯水泥体系相比,复合胶凝材料体系的化学结合水含量较低;化学结合水含量与抗压强度之间具有较好的线性相关性,但仅依靠化学结合水含量评价复合胶凝材料体系的强度发展仍有一定局限性,还需结合材料组成、反应活性和颗粒填充效应进行综合分析。研究成果可为工业固废资源化利用、低碳复合胶凝材料的配合比优化及性能调控提供参考。

Abstract:  The mechanical properties of cement-based materials are closely related to the degree of cement hydration. The chemically bound water method is a commonly used approach for quantitative characterization of the hydration degree in pure cement systems. However, when supplementary cementitious materials (SCMs) such as slag powder and fly ash are incorporated, the hydration process of the cementitious system becomes increasingly complex, and the traditional chemically bound water method cannot directly reflect the macroscopic mechanical properties of the composite system. To address this, this study employed cement, fly ash, slag powder, and quartz powder as raw materials, and designed one pure cement system and four composite cementitious material systems. The hydration mechanisms and mechanical property evolution were investigated, and the quantitative relationship between chemically bound water content and compressive strength was revealed. The results show that, compared with the pure cement system, the composite cementitious systems exhibit lower compressive strength. Overall, a reasonable combination of slag powder, fly ash, and quartz powder can improve the later-age compressive strength of the materials to a certain extent. The flexural strength of the composite cementitious system is sensitive to particle size distribution, matrix compactness, and crack propagation. Compared with the pure cement system, the composite cementitious systems have lower chemically bound water content. A good linear correlation is observed between chemically bound water content and compressive strength. However, relying solely on chemically bound water content to evaluate the strength development of composite cementitious material systems still has certain limitations, and comprehensive analysis should also take into account material composition, reaction activity, and particle packing effect. The findings can provide a reference for the resource utilization of industrial solid wastes, as well as for the mix proportion optimization and performance regulation of low-carbon composite cementitious materials. 

结论

(1)与P100纯水泥体系相比,各组复合胶凝材料体系的3、7、28 d抗压强度均较低,且不同复合胶凝材料体系的抗压强度发展规律存在差异,这主要与水泥含量、SCMs反应活性及颗粒填充效应有关。石英粉主要表现为惰性填充和稀释效应,矿渣粉可通过潜在水硬活性促进后期强度发展,粉煤灰早期反应活性较低,但在适当Ca(OH)2环境下可参与后期水化反应。总体而言,矿渣粉、粉煤灰与石英粉经合理复配后,可对水泥基材料后期抗压强度起到一定增益效果。
(2)与抗压强度相比,复合胶凝材料体系的抗折强度变化规律更加复杂,部分复合胶凝材料体系在特定龄期下表现出高于P100纯水泥体系的抗折强度,说明抗折强度对颗粒级配、基体密实性及裂缝扩展更为敏感,其发展规律与抗压强度不完全等同。
(3)复合胶凝材料体系的化学结合水含量随着龄期的增加而增大,3 d时化学结合水含量已达到28 d时的66.3%~76.3%,7 d时达到28 d时的81.8%~85.2%,说明胶凝材料体系的大部分水化反应主要发生在早期。
(4)P100纯水泥体系的化学结合水含量最高,P80Q20、P60S10Q30、P40F20S20Q20和P20F40S30Q10体系的化学结合水含量依次降低,说明复合胶凝材料体系的化学结合水含量受水泥含量、SCMs反应活性及惰性填料稀释效应共同影响。
(5)化学结合水含量与抗压强度之间具有较好的线性相关性,各体系相关系数R2均大于 0.940 0,说明化学结合水含量能够较好地反映同一胶凝材料体系的水化程度及抗压强度发展规律。
(6)P100纯水泥体系的拟合斜率最高,说明纯水泥体系中单位化学结合水含量增长对抗压强度发展的贡献较大。引入粉煤灰、矿渣粉和石英粉后,复合胶凝材料体系的拟合斜率降低,说明仅依靠化学结合水含量评价复合胶凝材料体系的强度发展具有一定局限性,还需结合材料组成、反应活性和颗粒填充效应进行综合分析。
(7)从工程应用角度来看,建立化学结合水含量与抗压强度之间的定量关系,有助于通过水化程度预测材料强度发展规律,为低碳复合胶凝材料的配合比优化及性能调控提供方法参考,并为工业固废资源化利用及绿色建筑材料开发提供参考。

参考文献

引用本文

冯发堂,王亚楠,钟益斌,等.低碳复合胶凝材料体系的力学性能与水化程度定量关系研究[J].混凝土与水泥制品,2026,53(10):52-57. Feng Fatang,Wang Yanan,Zhong Yibin,et al.Quantitative relationship between mechanical properties and hydration degree of low-carbon composite cementitious material systems[J].China Concrete and Cement Products,2026,53(10):52-57 (in Chinese).