全部文章
陈科技1,李国强1,成 智1,游秀菲2,曾 强2,*
陈科技,李国强,成智,等.风积沙-固废微粉复合高导热型电缆沟槽填充材料的制备与工程应用验证[J].混凝土与水泥制品,2026,53(10):99-105. Chen Keji,Li Guoqiang,Cheng Zhi,et al.Preparation and engineering application of aeolian sand-solid waste micropowder composite as high-thermal-conductivity cable trench backfill material[J].China Concrete and Cement Products,2026,53(10):99-105 (in Chinese).
何俊辉1,2,曲晓斌3,王 印3,明 阳4,*,景新臣3,安东升3,鹿重阳3,王文刚3, 梁崇博3,曹韩崇3,吴 飞3,任 昊4
何俊辉,曲晓斌,王印,等.多元固废超细复合掺合料改性UHPC的水化特性、收缩及抗侵蚀性能研究[J].混凝土与水泥制品,2026,53 (10):106-111. He Junhui,Qu Xiaobin,Wang Yin,et al.Study on hydration behavior, shrinkage and erosion resistance of UHPC modified by multi-component solid waste based ultrafine composite admixture[J].China Concrete and Cement Products,2026,53(10):106-111 (in Chinese).
章佩佳1,张荣富1,刘 俊1,李俊均1,杨东来1,司新秀2,3,王序晖2,3,曾思清3,4,张同生2,3,*
摘 要:为了降低蒸养混凝土资源消耗与碳排放量、推动废弃黏土砖高效资源化利用,本文采用超细再生砖粉(Ultra-fine recycled brick powder,UFRBP)等质量替代部分水泥制备了蒸养混凝土,研究了预养时间、升温和降温速率、蒸养温度、恒温时间及UFRBP掺量(0、10%、15%、20%)对蒸养混凝土抗压强度、耐久性能与微观结构的影响,并进行了经济与环境效益评价。结果表明:预养时间14 h、升降温速率10 ℃/h、蒸养温度60 ℃、恒温时间8 h为最优蒸养制度,同步掺入20%的UFRBP时,混凝土的7 d抗压强度达到最大,抗氯离子渗透性能最好;UFRBP在蒸养条件下充分发挥了微集料填充效应与火山灰效应,细化了混凝土孔结构,优化了界面过渡区性能,从而显著改善了混凝土的宏观性能;相较于采用传统蒸养制度的纯水泥混凝土,采用优化蒸养制度并掺入20%的UFRBP混凝土的生产能耗、生产成本、碳排放、自然资源消耗均显著降低,经济和环境效益显著。研究成果可为UFRBP在蒸养混凝土中的高效、绿色工程应用提供参考。Abstract: To reduce resource consumption and carbon emissions in the production of steam curing concrete and to promote the high-efficiency resource utilization of waste clay bricks, this study prepared steam curing concrete by replacing a portion of cement with ultra-fine recycled brick powder (UFRBP) at equivalent mass ratios. The effects of pre-curing time, heating and cooling rates, steam curing temperature, isothermal holding time, and UFRBP contents (0, 10%, 15%, and 20%) on the compressive strength, durability, and microstructure of steam curing concrete were systematically investigated, accompanied by an economic and environmental benefit assessment. The results indicate that the optimal performance is achieved under a steam curing regime with a pre-curing time of 14 h, heating and cooling rates of 10 ℃/h, a steam curing temperature of 60 ℃, and an isothermal holding time of 8 h, in combination with a UFRBP content of 20%. Under these conditions, the concrete attains its maximum 7-day compressive strength and exhibits the best resistance to chloride penetration. Under steam curing conditions, UFRBP fully exerts both its microfiller effect and pozzolanic activity, which refine the pore structure and improve the interfacial transition zone performance, thereby significantly enhancing the macroscopic properties of the concrete. Compared with plain cement concrete subjected to a conventional steam curing regime, the concrete incorporating 20% UFRBP under the optimized regime exhibits substantially lower energy consumption, production cost, carbon emissions, and natural resource depletion, demonstrating significant economic and environmental benefits. The findings can provide a valuable reference for the efficient and green engineering application of UFRBP in steam curing concrete.
章佩佳,张荣富,刘俊,等.蒸养制度和超细再生砖粉协同调控蒸养混凝土性能及双效益分析[J].混凝土与水泥制品,2026,53(10):72-79. Zhang Peijia,Zhang Rongfu,Liu Jun,et al.Synergistic regulation of steam curing concrete performance by steam curing regime and ultra-fine recycled brick powder and its dual benefits[J].China Concrete and Cement Products,2026,53(10):72-79 (in Chinese).